Problems and improvement measures in the manufacturing process of copper bars
Release time:2023-09-06Click:790
At present, the production characteristics of copper bars in China are short process, high yield, and environmentally friendly. There are some common problems in the manufacturing process of copper bars:
1. Problem with the pole
The oxygen content exceeds the standard, and even there are pores (oxygen content f oxygen free copper ≤ 10ppm)
Coarse and loose grainsCold shut and surface cracks
Surface oxidation (temperature above 100 ℃ forms black copper oxide, temperature above 180 ℃ forms orange red cuprous oxide, temperature above 400 ℃ accelerates oxidation, and oxidation rate increases with increasing humidity)
2. Problems with soft volleyball
Surface and internal bubbles
Scratches and oxidation
Narrow edge cracks (large soft fill defects)
3. Problems with hard copper bars
Copper bar oxidation (orange or black)
Uneven size of copper bars
Surface defects (spots, pits, scratches, color differences, and defects) of copper bars
4. Tin coating issues
Blackening of tin coating (oxidation of Sn coating)
Measures to improve the quality of copper bars
1. Measures for improving the quality of copper rods
Purify raw materials and auxiliary materials, reduce oxygen content (remove copper beans and copper green; screen and dry charcoal and graphite sheets; dry utensils)
During smelting, copper should not be exposed at the furnace mouth, and charcoal should be covered in place (≥ 10-15cm) to reduce oxygen content
Regularly clean the slag hanging at the furnace mouth to reduce inclusions
Control the temperature and temperature fluctuation of copper liquid, reduce oxygen content, avoid eliminating looseness and cold insulation (≤ 1150 ℃), high temperature, high gas content, low temperature, and poor fluidity
Strictly control the rod making process, control the temperature of the cooling water in the crystallizer (the inlet temperature should not be higher than 30 ℃, and the difference in inlet and outlet water temperature should be controlled within 10-15 ℃), pressure, flow rate, and rod speed to prevent the occurrence of hollow rods, coarse grains, loose structures, and oxidation
Occasional spot checks (oxygen content analysis, or 820 ℃) × 20 min annealing,)
Copper liquid deoxygenation treatment and grain refinement treatment
2. Measures for improving the quality of soft discharge
Eliminate bubbles, control the oxygen content and surface state (oxidation, oil stains, dust, and water stains) of oxygen free copper rods; It is strictly prohibited to bring in gas during the extrusion process (damage to the surface of the copper rod, leakage of cooling water from the extrusion wheel, damage and wrinkling of the copper clad area in the groove of the extrusion wheel, and waste material brought into the extrusion wheel)
Eliminate scratches, polish the surface of the extrusion mold, and ensure the smoothness of the sizing belt; Varying the extrusion speed to remove the oxide attached to the sizing strip
Eliminate oxidation, increase cooling speed, add 3-8% alcohol to the coolant, or use lubricating agent liquid+water
Narrow edge cracks improve metal fluidity (cavity preheating in place, 700-800 ℃ × 10 minutes, appropriately lengthen the length of the mold sizing belt to increase the extrusion driving force,
Optimize extrusion parameters, control recrystallization, and refine grain size
3. Measures for improving the quality of copper bars
Control the unevenness of the thickness of the copper busbar soft busbar to reduce the bending deformation of the hard copper busbar
Water soluble stretching oil lubricates the stretching mold (reduces scratches and scratches, improves smoothness and accuracy)
After stretching, let it stand for a period of time before stacking to avoid oxidation (if the temperature is higher than 100 ℃, black copper oxide will form;)
Standardized packaging (reducing bumps and static electricity during transportation)
Improvement of drawing molds and lubrication cooling fluid, as well as automated testing
4. Improvement of tin coating quality
Control the purity of Sn
Strengthen the cold and hot water cleaning treatment of electroplating tin
Improve storage environment, seal after tin plating and drying
New requirements for adding anti oxidation film copper bars
Solve the issue of adding furnace feed
Reducing the Contact Resistance of Copper Bars
New Technology for Developing High Conductivity and High Extension New Copper Bars and Copper Bars
Copper liquid degassing and impurity removal technology
Grain Refinement Technology for Copper Rod and Copper Strip
Copper bar bright technology
Anti oxidation Technology of Copper Bar Tin Plating Layer
Surface passivation treatment technology for copper bars
Article source: Internet
Disclaimer: Some pictures and texts on this site are collected from the Internet and are only for learning and communication. The copyright belongs to the original author and does not represent the views of our site. This site will not bear any legal responsibility. If your rights are violated, please contact us to delete it in time.